Table 8

Main results for the polylactic acid plasticized samples manufactured by additive manufacturing with longitudinal pattern

Referenceθ0 (°)θ300(°)Rr (%)
PLA-L178.6 ± 0.572.5 ± 1.759.4 ± 1.0
10TEC-L178.5 ± 0.4126.5 ± 0.629.1 ± 0.4
20TEC-L166.0 ± 0.8154.0 ± 2.27.2 ± 1.5
10TEC/PLA/10TEC-L178.3 ± 1.0104.8 ± 0.741.2 ± 0.4
20TEC/PLA/20TEC-L114.5 ± 1.343.0 ± 0.862.4 ± 0.3
PLA/10TEC/PLA-L177.0 ± 0.879.0 ± 0.855.4 ± 0.7
20TEC/10TEC/20TEC-L103.0 ± 0.862.5 ± 0.639.3 ± 0.7
PLA/20TEC/PLA-L177.3 ± 1.032.8 ± 1.081.5 ± 0.6
10TEC/20TEC/10TEC-L159.0 ± 0.842.4 ± 0.473.3 ± 0.4
Source(s): Authors’ own work