LPBF process parameters and number of remelts used for processing of blended elemental Ni and Ti powders
| Platform no. | Remelting no. | Melting | 1st remelting | 2nd remelting |
|---|---|---|---|---|
| 1 | Single melting (SM) | 14–80 J/mm3 (P = 25–30W, v = 500–1,000 mm/s) | ||
| 2 | Single melting (SM) + one remelting | 14–80 J/mm3 (P = 25–30 W, v = 500–1,000mm/s) | 33 J/mm3 (R1) (P = 25 W, v = 1,000mm/s) | |
| 3 | Single melting (SM) + two remeltings | 14–80 J/mm3 (P = 25–30 W, v = 500–1,000mm/s) | 33 J/mm3 (R1) (P = 25 W, v = 1,000mm/s) | 33 J/mm3 (R1) (P = 25 W, v = 1,000mm/s) |
| 4 | Single melting (SM) + one remelting | 14–80 J/mm3 (P = 25–30 W, v = 500–1,000mm/s) | 33 J/mm3 (R2) (P = 75 W, v = 3,000mm/s) | |
| 5 | Single melting (SM) + two remeltings | 14–80 J/mm3 (P = 25–30 W, v = 500–1,000mm/s) | 33 J/mm3 (R2) (P = 75 W, v = 3,000mm/s) | 33 J/mm3 (R2) (P = 75 W, v = 3,000mm/s) |
| Remelting no. | Melting | 1st remelting | 2nd remelting | |
|---|---|---|---|---|
| Single melting (SM) | 14–80 J/mm3 | |||
| Single melting (SM) + one remelting | 14–80 J/mm3 | 33 J/mm3 (R1) | ||
| Single melting (SM) + two remeltings | 14–80 J/mm3 | 33 J/mm3 (R1) | 33 J/mm3 (R1) | |
| Single melting (SM) + one remelting | 14–80 J/mm3 | 33 J/mm3 (R2) | ||
| Single melting (SM) + two remeltings | 14–80 J/mm3 | 33 J/mm3 (R2) | 33 J/mm3 (R2) |